| AL2O3% Composition |
Density
(g/cm3) |
Flexural Strength
(MPa) |
Thermal Conductivity
[w/(m.R)] |
Dielectric Strength
(KV/mm) |
Working Temp. |
| 60 | 3.0 | 205 | 16 | 10 | 1000°C |
| 75 | 3.1 | 280 | 17 | 10 | 1250°C |
| 80 | 3.3 | 215.7 | 17 | 10 | 1290°C |
| 85 | 3.4 | 230 | 17 | 10 | 1350°C |
| 92 | 3.6 | 312 | 18 | 10 | 1390°C |
| 95 | 3.7 | 304 | 20 | 10 | 1480°C |
| 99 | 3.81 | 340 | 34 | 10 | 1600°C |
| 99.7 | 3.85 | 370 | 35 | 10 | 1700°C |
|
Al2O3 content
% |
70-75 | 85 | 95 | 99.7 |
|
Density
(g/cm3) |
3.0 | 3.4 | 3.7 | 3.9 |
|
Bending Strength
(Mpa) |
85N/MM2 | 300 | 364 | 450 |
|
Expansion
(X10-6/°C)(25-800°C) |
6 | 7 | 7.6 | 8 |
|
Thermal Conductivity
(W/(m.R)) |
17 | 18 | 20 | 35 |
|
Dielectric Strength
(kv/mm) |
9 | 10 | 11 | 12 |
|
Working Temperature
°C (Long time use) |
1300 | 1400 | 1600 | 1750 |
|
Water Absorption
% |
5 | <0.2 | <0.2 | <0.1-0.2 |
| Characteristics | Items | Types | |||
| VS-2000 | S-2000 | S-4000 | S-6000 | ||
|
Physical
properties |
Bulk density ( g/cm3 ) | ≥2.4 | ≥2.4 | ≥2.6 | ≥2.8 |
| Apparent porosity ( % ) | 20-23 | 20-25 | 15-20 | 10-15 | |
| Water absorption ( % ) | 8-10 | 8-12 | 7-10 | 4-7 | |
|
Bending strength
(25 ºC /1350 ºC ,Mpa ) |
>55/35 | >50/30 | >60/50 | >70/60 | |
|
Thermal expansion coefficient
(*10(-6)/ ºC )(25~1000 ºC ) |
5.8-6.0 | 5.8-6.2 | 5.8-6.2 | 5.8-6.0 | |
| Thermal shock resistance ( 1300~25 ºC ) | Good | Very good | Very good | Good | |
| Working Temp ( ºC ) | ≤1200 | ≤1230 | ≤1300 | ≤1350 | |
| Composition | Al2O3(5) | 74-76 | 74-76 | 72-74 | 78-80 |
| SiO2(%) | 20-22 | 20-22 | 19-21 | 14-16 | |
| Fe2O3(%) | ≤0.3 | ≤0.3 | ≤0.3 | ≤0.2 | |
|
Reference
loading |
Φ50*3800mm |
5.0
(1200 ºC ) |
4.5
(1230 ºC ) |
6.0
(1300 ºC ) |
7.5
(1350 ºC ) |