| C | Si | Mn | P | S | Cr | Mo | W | V | Co | Ni |
|---|---|---|---|---|---|---|---|---|---|---|
| 0,36-0,42 | Max 1,00 | Max 1,00 | Max 0,030 | Max 0,030 | 12,50-14,50 | - | - | - | - | - |
| Hardness after | Tempering ºC | Symbol | Value |
| Soft annealing | - | HB | ≤241 |
| Toughening | HB | 300 | |
| Quenching with 1010 ºC in oil | - | HRC | 54 |
|
Quenching with 1010 ºC in oil and tempering
(cooling during quenching can also be performed either in the air or gradually in the salt bath at 500-550 ºC and then cooled in the air) |
180 | HRC | ≥52 |
| 200 | HRC | 53 | |
| 250 | HRC | 52.5 | |
| 450 | HRC | 54 | |
| 500 | HRC | 52.5 | |
| 550 | HRC | 49.5 | |
| 600 | HRC | 46 |
| Property | Unit | Value |
| Density, ρ | g*cm -3 | 7.60 |
| Thermal expansion, α 20-100ºC) | K -1 | 10.6*10 -6 |
| Thermal conductivity, λ 20ºC) | W*m -1 *K -1 | 29 |
| Technological treatment processes | Possible application | Temperature, °C | ||
| Hot forming | Forging | + | 1100-800 | |
| Rolling | + | 1100-800 | ||
| Treatment | Heat treatment | Quenching | + | 1000-1050 |
| Tempering | + |
150-300
400-600 |
||
| Precipitation strengthening | Supersaturation | - | - | |
| Ageing | - | - | ||
| Annealing | Soft annealing | + | 750-800 | |
| Stress relieving | + | 600-700 | ||
| Thermochemical treatment | Nitriding | + | 470-520 | |
| Other | - | - | ||
| ISO | CEN | Russia | |||
| X40Cr14 | ISO 4957:2004 | X40Cr14 | ISO 4957:2004 | - | - |
| US | Japan | China | |||
| - | - | - | - | - | - |