| C | Si | Mn | P | S | Cr | Mo | W | V | Co | Ni |
|---|---|---|---|---|---|---|---|---|---|---|
| 1,20-1,35 | Max 0,45 | - | Max 0,030 | Max 0,030 | 3,80- 4,50 | 3,20-3,90 | 9,00-10,00 | 3,00-3,50 | 9,50-10,50 | - |
| Hardness after | Tempering ºC | Symbol | Value |
| Soft annealing | - | HB | ≤302 |
| Quenching with 1230 ºC in oil | - | HRC | 66 |
| Quenching with 1230 ºC in oil and tempering (cooling during quenching can be gradual in the salt bath at the temperature of around 550 ºC and then in the air) | 350 | HRC | 61 |
| 400 | HRC | 62 | |
| 450 | HRC | 64 | |
| 500 | HRC | 66 | |
| 550 | HRC | 66.5 | |
| 600 | HRC | 65 | |
| 650 | HRC | 62 | |
| 700 | HRC | 55 |
| Property | Unit | Value |
| Density, ρ | g*cm -3 | 8.30 |
| Technological treatment processes | Possible application | Temperature, °C | ||
| Hot forming | Forging | + | 1050-900 | |
| Rolling | + | 1050-900 | ||
| Heat treatment | Soft annealing | + | 800-900 | |
| Stress relieving | + | 600-700 | ||
| Quenching | Heating I | + | ~550 | |
| Heating II | + | 850 | ||
| Austenitising | + | 1190-1240 | ||
| Tempering | + | 550-600 | ||
| Surface treatment | Nitriding | + | 510-550 | |
| Coat application | + | PVD | ||
| ISO | CEN | Russia | |||
| HS10-4-3-10 | ISO 4957:2004 | HS10-4-3-10 | ISO 4957:2004 | - | - |
| US | Japan | China | |||
| - | - | ~SKH 57 | JIS G 4403-1983 | - | - |